CARBON TOUGHENING STEEL
NORM: PN/EN 10083-2
APPLICATION:
Steel susceptible to the parts averagely exposed on loadings and more resistant to abrasion. For the parts such as: axles, crankshafts, spindles, discs, pump rotors, etc.
TECHNOLOGICAL INFORMATION:
After soft annealing, steel becomes machinable; if normalised and soft annealed, steel becomes adjusted for the mechanical cutting.
SEMI-FINISHED PRODUCTS:
After soft annealing, steel becomes machinable; if normalised and soft annealed, steel becomes adjusted for the mechanical cutting.
CHEMICAL COMPOSITION:
C | Mn | Si | P | S | Cr | Ni | Mo | V | W | Ti | Cu | Inne |
---|---|---|---|---|---|---|---|---|---|---|---|---|
0,42 - 0,50 | 0,50 - 0,80 | Max 0,40 | Max 0,045 | Max 0,045 | Max 0,40 | Max 0,40 | Max 0,10 | - | - | - | - | Cr+Mo+Ni max 0,63 |
MECHANICAL PROPERTIES:
Effect of the cross-section on mechanical properties | |||
If heat treated | |||
Diameter d, mm
Thickess of the flat bar t, mm |
≤ 16
≤ 8 |
16–40
8–20 |
40–100
20–60 |
Ultimate tensile strength Rm, MPa | 700–850 | 650–800 | 630–780 |
Yield stress Re (Rp0.2), MPa | ≥ 490 | ≥ 430 | ≥ 370 |
Elongation, A, % | ≥ 14 | ≥ 16 | ≥ 17 |
Reduction of area, Z, % | ≥ 35 | ≥ 40 | ≥ 45 |
If normalised | |||
Diameter, d, mm
Thickness of the flat bar t, mm |
≤ 16
≤ 16 |
16–100
16–100 |
100–250
100–250 |
Ultimate tensile strength Rm, MPa | ≥ 620 | ≥ 580 | ≥ 560 |
Yield stress Re (Rp0.2), MPa | ≥ 340 | ≥ 305 | ≥ 275 |
Elongation, A, % | ≥ 14 | ≥ 16 | ≥ 16 |
Technological treatment processes:
Technological treatment processes | Possible application | Temperature, °C | ||
Hot forming | Forging | + | (1100 – 850) | |
Rolling | + | (1100 – 850) | ||
Treatment | Heat treatment | Quenching | + | 820-860/w,o |
Tempering | + | 550 – 660 | ||
Precipitation strengthening | Supersaturation | – | – | |
Ageing | – | – | ||
Annealing | Normalising | + | 840 – 900 | |
Soft annealing | + | (650 – 700) | ||
Thermochemical treatment | Carburising | – | – | |
Other | – | – |
INTERNATIONAL STEEL GRADES:
ISO | EN | Russia | |||
~C45 | ISO 683-1 1987 | C45 | EN 10083-2 1996 | ~ 45 | GOST 1050 1988 |
US | Japan | China | |||
~ M 1044 | ASTM A 29-93 | ~S 45 C | JIS G 4051 1979 | ~ 45 | GB 699-88 |