CARBON TOUGHENING STEEL

NORM: PN/EN 10083-2

APPLICATION:

Steel susceptible to the parts averagely exposed on loadings and more resistant to abrasion. For the parts such as: axles, crankshafts, spindles, discs, pump rotors, etc.

TECHNOLOGICAL INFORMATION:

After soft annealing, steel becomes machinable; if normalised and soft annealed, steel becomes adjusted for the mechanical cutting.

SEMI-FINISHED PRODUCTS:

After soft annealing, steel becomes machinable; if normalised and soft annealed, steel becomes adjusted for the mechanical cutting.

CHEMICAL COMPOSITION:

CMnSiPSCrNiMoVWTiCuInne
0,42 - 0,500,50 - 0,80Max 0,40Max 0,045Max 0,045Max 0,40Max 0,40Max 0,10----Cr+Mo+Ni max 0,63

MECHANICAL PROPERTIES:

Effect of the cross-section on mechanical properties
If heat treated
Diameter d, mm

Thickess of the flat bar t, mm

≤ 16

≤ 8

16–40

8–20

40–100

20–60

Ultimate tensile strength Rm, MPa 700–850 650–800 630–780
Yield stress Re (Rp0.2), MPa ≥ 490 ≥ 430 ≥ 370
Elongation, A, % ≥ 14 ≥ 16 ≥ 17
Reduction of area, Z, % ≥ 35 ≥ 40 ≥ 45
If normalised
Diameter, d, mm

Thickness of the flat bar t, mm

≤ 16

≤ 16

16–100

16–100

100–250

100–250

Ultimate tensile strength Rm, MPa ≥ 620 ≥ 580 ≥ 560
Yield stress Re (Rp0.2), MPa ≥ 340 ≥ 305 ≥ 275
Elongation, A, % ≥ 14 ≥ 16 ≥ 16

Technological treatment processes:

Technological treatment processes Possible application Temperature, °C
Hot forming Forging + (1100 – 850)
Rolling + (1100 – 850)
Treatment Heat treatment Quenching + 820-860/w,o
Tempering + 550 – 660
Precipitation strengthening Supersaturation
Ageing
Annealing Normalising + 840 – 900
Soft annealing + (650 – 700)
Thermochemical treatment Carburising
Other

INTERNATIONAL STEEL GRADES:

ISO European Union Russia
~C45 ISO 683-1 1987 C45 EN 10083-2 1996 ~ 45 GOST 1050 1988
US Japan China
~ M 1044 ASTM A 29-93 ~S 45 C JIS G 4051 1979 ~ 45 GB 699-88