TOUGHENING STEEL

NORM: PN/EN 10083-3

Anmeldung:

Steel with a standard tensile strength and a good weldability. Steel susceptible for automotive and aircraft components with high toughness such as axles, axle journals, turbine parts, turbine rotors.

TECHNOLOGISCHE INFORMATIONEN::

After soft annealing steel becomes machinable ( by improved shearability) and adjusted for the mechanical cutting.

Zwischenprodukte:

After soft annealing steel becomes machinable ( by improved shearability) and adjusted for the mechanical cutting.

Chemische Zusammensetzung:

CMnSiPSCrNiMoVWTiCuInne
0,22 - 0,290,60 - 0,90Max 0,40Max 0,025Max 0,0350,90 - 1,20-0,15 - 0,30-----

Mechanische Eigenschaften:

Mechanical properties of a product with diameter d ≤ 16 mm
Property Symbol Unit After heat treatment
Ultimate tensile strength Rm MPa 900–1100
Yield stress Re (Rp0.2) MPa ≥ 700
Elongation A % ≥ 12
Reduction of area Z % ≥ 50
Impact energy KV J ≥ 45
The influence of the element’s cross-section on mechanical properties
Diameter d, mm

Thickness of the flat bar t, mm

16–40

8–20

40–100

20–60

100–160

60–100

Rm, MPa 800–950 700–850 650–800
Re (Rp0.2), MPa ≥ 600 ≥ 450 ≥ 400
A, % ≥ 14 ≥ 15 ≥ 16
Z, % ≥ 55 ≥ 60 ≥ 60
KV, J ≥ 50 ≥ 50 ≥ 45

Technologische Verarbeitung:

Technological treatment processes Possible application Temperature, °C
Hot forming Forging + (1050–850)
Rolling + (1180–850)
Treatment process Heat treatment Quenching + 840–900/w,o
Tempering + 540–680
Precipitate strengthening Supersaturation
Ageing
Annealing Normalising + (860–900)
Soft annealing + (680–720)
Thermochemical treatment Carburising
Other

INTERNATIONALE STAHLSORTEN:

ISO European Union Russia
25CrMo4 ISO 683-1 1987 25CrMo4 EN 10083-1 1996 ~20ChM

~30ChM

GOST 4543 1971
US Japan China
~ 4130 ASTM A 322-91 ~SCM2

~SCM22

JIS G 4105 1979 ~30CrMo GB 3077-88