50HF/1.8159/51CrV4

SPRING STEEL

NORM: PN-EN 10132-4

APPLICATION:

Steel susceptible to parts for general mechanical engendering, axles, shafts, automotive and gear parts, crankshafts, connecting-rods of engines; surface hardened for parts with high strength cores

TECHNOLOGICAL INFORMATION:

After soft annealing steel becomes machinable ( by improved shearability) and adjusted for the mechanical cutting.

SEMI-FINISHED PRODUCTS:

After soft annealing steel becomes machinable ( by improved shearability) and adjusted for the mechanical cutting.

CHEMICAL COMPOSITION:

CMnSiPSCrNiMoVWTiCuInne
0,47 - 0,550,70 - 1,10Max 0,40Max 0,025Max 0,0250,90 - 1,20--0,10 - 0,25----

MECHANICAL PROPERTIES:

Mechanical properties of a product with the diameter d ≤ 16 mm
Property Symbol Unit After heat treatment
Ultimate tensile strength Rm MPa 1100-1300
Yield stress Re (Rp0,2) MPa ≥ 900
Elongation A % ≥ 9
Reduction of area Z % ≥ 40
Impact energy KV J ≥ 30
Effect of the cross-section on mechanical properties
Diameter d, mm

Thickness of the flat bar t, mm

16 – 40

8 – 20

40 – 100

20 – 60

100 – 160

60 – 100

160 – 250

100 – 160

Rm, MPa 1000 – 1200 900 – 1100 850 – 1000 800 – 950
Re (Rp0,2), MPa ≥ 800 ≥ 700 ≥ 650 ≥ 600
A, % ≥ 10 ≥ 12 ≥ 13 ≥ 13
Z, % ≥ 45 ≥ 50 ≥ 50 ≥ 50
KV, J ≥ 30 ≥ 30 ≥ 30 ≥ 30

Technological treatment processes:

Technological treatment processes Possible application Temperature, °C
Hot forming Forging + (1050 – 850)
Rolling + (1180 – 850)
Treatment Heat treatment Quenching + 820-870/w,o
Tempering + 540 – 680
Precipitation hardening Supersaturation
Ageing
Annealing Normalising + (850 – 880)
Soft annealing + (640 – 680)
Thermochemical treatment Carburising
Other

INTERNATIONAL STEEL GRADES:

ISO European Union Russia
51CrV4 ISO 683-1 1987 51CrV4 EN 10083-1 1996 ~ 50ChFA GOST 14959 1979
US Japan China
~6150H ASTM A 304-95 SUP 10 JIS G 4801 1984 50CrVA GB 8162-87